Preparation of crown ether complexing highly active double metal cyanide catalysts and copolymerization of CO2 and propylene oxide
Min Zhanga , Yong Yangb,c, Liban Chenb    
a College of Food and Horticultural Sciences, Foshan University, Foshan 528231, Guangdong, China;
b Guangzhou Institute of Chemistry, Chinese Academy of Sciences, Guangzhou 510650, Guangdong, China;
c University of Chinese Academy of Sciences, Beijing 100049, China
Abstract: Double metal cyanide (DMC) catalysts are generally prepared by coprecipitation of potassium hexacyanocobaltate(III) with zinc chloride followed by complexation with tert-butanol, and these materials have been used for several decades in the copolymerization of CO2 and epoxides. However, the catalytic efficiency of DMC catalysts can be adversely affected by the presence of excess K+, and the preparation of these catalysts can therefore become complicated and time-consuming because of the multiple washing and centrifugation stages required for the removal of the excess K+. In this study, 18-crown-6 ether was used as an effective co-complexing agent for the removal of K+. A series of DMCs containing 18-crown-6 were prepared with different quantities of the crown ether and different washing times. The resulting crown ether-complexing catalysts (CDMCs) and DMC catalysts without crown ether were characterized by Fourier transform infrared spectroscopy, scanning electron microscopy, thermogravimetric analysis-IR and X-ray diffraction. These characterization results showed that the inclusion of 18-crown-6 allowed for the formation of uniform and highly dispersed CDMC catalysts. In contrast, the DMC catalysts prepared in the absence of 18-crown-6 became uneven and delaminated during the purification by centrifugation, with high- and low-density portions of the material forming on the bottom and top of the catalyst cakes, respectively. The inclusion of 18-crown-6 not only trapped K+ but also participated in the complexion process. The complexion of tert-BuOH and 18-crown-6 led to a less crystalline form of the CDMC catalyst. Elemental analysis revealed that CDMC1 contained 1.2% K+. The copolymer was obtained by the copolymerization of CO2 with propylene oxide using CDMC3 catalyst, which was superior to the copolymer prepared using DMC1. CDMC3 was as active as DMC2 prepared without the crown ether but with seven washing steps. A hypothetical two-stage catalytic mechanism was proposed.
© 2015, Dalian Institute of Chemical Physics, Chinese Academy of Sciences.
Published by Elsevier B.V. All rights reserved.
Key words: Double metal cyanide     Carbon dioxide     Propylene oxide     Copolymerization     Crown ether    
冠醚络合高活性双金属氰化物制备及CO2与环氧丙烷共聚
张敏a , 杨永b,c, 陈立班b    
a 佛山科学技术学院食品与园艺学院, 广东佛山528231;
b 中国科学院广州化学研究所, 广东广州510650;
c 中国科学院大学, 北京100049
摘要:首次在共沉淀过程中添加18-冠-6醚络合生成的钾离子得到了均一的高活性冠醚络合的锌-钴双金属催化剂, 并用红外光谱(FTIR)、扫描电镜(SEM)、热重红外(TGA-IR)和X射线衍射(XRD)进行了表征. 元素分析发现K含量为1.2%. FTIR表明未加冠醚络合的双金属催化剂离心后上下部分呈现不同的络合状态, 而冠醚络合的双金属催化剂仍保持均一. SEM表明冠醚络合的双金属催化剂为均一松散的结构. 由于生成的钾离子被冠醚络合, 不影响聚合反应效果. TGA-IR表明冠醚不仅络合K离子, 还参与对金属活性中心的络合. XRD表明此催化剂具有低的结晶度. 所制冠醚络合的锌-钴双金属催化剂能成功催化CO2与环氧丙烷共聚, 其中CDMC3催化得到的共聚物碳酸酯含量为47.8%, 副产物环状碳酸酯为1.5%, 催化效率高达5122 g/g催化剂(32600 g/g Zn), 明显优于不添加冠醚以同样工艺制备的DMC1 (共聚物碳酸酯含量29.2%, 副产物环状碳酸酯3.3%, 催化效率4100 g/g催化剂(16300 g/g Zn). 与不添加冠醚8次洗涤离心得到的DMC2相当(共聚物碳酸酯含量48.3%, 副产物环状碳酸酯含量2.4%, 催化效率5073 g/g催化剂(16400 g/g Zn)). 基于此结果提出了两步的反应机理假设.
关键词双金属氰化物     二氧化碳     环氧丙烷     共聚     冠醚    

1. Introduction

CO2, which is widely known as one of the main greenhouse gases, could potentially be used as building block for the construction of useful aliphatic polycarbonates. Aliphatic polycarbonates are becoming increasingly important because of their extensive range of applications in the production of polyurethanes, coating materials, biodegradable surfactants and biomedical materials [1, 2]. Aliphatic polycarbonates are mainly prepared by transesterification [3] and CO2 coupling [4] reactions. A wide variety of catalytic systems have been developed during the last three decades for the efficient copolymerization of CO2 with epoxides, including ZnEt2-protic compounds [5, 6], zinc glutarate or adipate [7, 8, 9], rare-earth catalysts [10, 11, 12], metal-porphyrins [13, 14, 15], zinc bis(β-diiminates) [16, 17, 18], salen-metal systems, metal microporous polymers [19, 20, 21, 22, 23, 24, 25] and double metal cyanide (DMC) catalysts [26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37]. DMC catalysts in particular have promising industrial prospects because of their high activity, cost-effectiveness and insensitivity to moisture.

DMC catalysts were initially used in the production of polyether and later utilized in the copolymerization of propylene oxide with CO2 [24, 25, 26, 27, 28, 29, 30]. DMC catalysts are typically prepared via a precipitation process with a heavy organic complexing agent such as tert-butyl alcohol (t-BuOH), followed by multiple washing and centrifugation stages to allow for the removal of the excess potassium ions [26, 27, 28, 29], which can have an adverse impact on the copolymerization of CO2 and propylene oxide [29]. A new process was recently developed to avoid the production of K+ where H3Co(CN)6 was prepared according to an ion exchange method using K3Co(CN)6, followed by precipitation with ZnCl2 in methanol to give [ZnCl]+2[HCo(CN)6]2- without any K+ [29]. This material was subsequently used in the copolymerization of CO2 with propylene oxide to give a copolymer product with a high molar fraction of CO2 (about 60%). Sebastian et al. [30] prepared a series of Zn-Co DMC catalysts with K+ contents in the range of 0.41%-2.0% without the inclusion of an additional washing step. However, the highest catalytic efficiency achieved with these Zn-Co DMC catalysts for the copolymerization of CO2 and cyclohexene oxide was only 52.8 g polymer/g catalyst. In light of the problems posed by the presence of K+ in these catalysts, significant research efforts have been directed towards the development of new techniques for the removal of free potassium ions from heterogeneous DMC catalysts. However, the traditional methods for the preparation of DMC catalysts require multiple washing and centrifugation (up to seven times), making these processes time consuming, inefficient and poorly reproducible [26, 27, 28, 31, 32].

It is noteworthy that 18-crown-6 ether has an appropriate hole size (0.26-0.32 nm) for the binding of K+ (0.266 nm). Herein, we describe the results of our study towards the preparation of DMC catalysts in the presence of 18-crown-6 with the aim of simplifying the washing and centrifugation steps. The resulting crown ether complexing Zn-Co DMC catalysts were subsequently evaluated as catalysts for the copolymerization of CO2 with propylene oxide.

2. Experimental
2.1. Materials

Potassium hexacyanocobaltate(III), 18-crown-6, zinc chloride and tert-butyl alcohol were purchased as the analytical grade from Aladdin Reagent (Shanghai, China) and used without further purification. Propylene oxide was refluxed over calcium hydride and then stored over 3Å molecular sieves prior to being used in the copolymerization reactions. CO2 (>99.9%) was purchased from Kedi Air Chmical (Foshan, China) and used without further purification.

2.2. Preparation of the catalysts

The methods used for the preparation of the catalysts are summarized in Table 1. CDMC1 was prepared according to Ref. [28, 32] with minor modifications. Briefly, a solution of K3[Co(CN)6] (1.66 g, 5 mmol) in distilled H2O (25 mL) was added in a dropwise manner to a vigorously stirred suspension of ZnCl2 (2.5 g, 18.4 mmol) in a mixture of distilled H2O (75 mL) and t-BuOH (40 mL) at 45 °C over 30 min, and the resulting mixture was stirred for 2 h. 18-Crown-6 (8 g, 30.3 mmol) was then added to the reaction in a single portion, and the resulting mixture was stirred for 3 h to allow for the complete complexation of the K+ ions. The resulting white precipitate was isolated by centrifugation (25 °C, 15 min), suspended in t-BuOH (140 ml) and stirred for 2 h at 45 °C. The mixture was then purified by centrifugation (25 °C, 15 min) to give the catalyst, which was dried under vacuum at 50 °C to constant weight, resulting in a cake. The top and bottom portions of the CDMC1 cake were labeled as CDMC1-T and CDMC1-B, respectively. All of the other catalysts prepared were defined in a similar manner. Elemental analysis of CDMC1 revealed 21.6% Zn, 8.1% Co and 1.2% K.

Table 1
Conditions used for the preparation of the different DMC catalysts a.

CDMC2 and CDMC3 were prepared according to a procedure similar to CDMC1 but with different crown ethers and washing times with a 1:1 (v/v) mixture of t-BuOH and water.

DMC1 and DMC2 were synthesized according to a similar procedure to that used for CDMC 1 but without addition of the crown ether [28, 32]. In the case of DMC2, the remaining K+ ions were removed by washing the precipitate seven times with a mixture of distilled H2O and t-BuOH whilst decreasing the quantity of H2O and increasing the amount of t-BuOH. Elemental analyses revealed the following results: DMC1 (Zn 25.14%, Co 8.53%, K 1.43%); DMC2 (Zn 30.85%, Co 9.81%, no K+ ions were detected). DMC0 consisted of pure Zn3[Co(CN)6]2, which was prepared in the absence of a complexing agent.

2.3. Catalyst characterization

Fourier transform infrared spectra (FTIR) were measured on an Analect RFX-65A FTIR spectrophotometer (Analect, USA). The surface morphologies of the DMC catalysts were observed by scanning electron microscopy (SEM) on a JSM-6360LV scanning electron microscope (JEOL, Japan). Prior to scanning, the top and bottom portions of the DMC and CDMC cakes were coated with a thin layer of gold under high vacuum conditions. X-ray powder diffraction (XRD) patterns were collected on a Bruker D8 Advance diffractometer (Bruker, Sweden) using monochromated radiation. The chemical compositions of the catalysts were obtained by elemental analysis using a Vario EL CHNS elemental analyzer (Elementar, Germany) equipped with a PE5100 ICP-AES instrument (Perkin Elmer, USA). A Thermogravimetric analysis/infrared spectra (TGA-IR) were recorded on a TG-209/VectorTM-22 system (Netzsch, Germany). 1H-NMR spectra of the copolymers were recorded on a DRX-400 spectrometer (400 MHz) using CDCl3 as a solvent. The molecular weights and molecular weight distributions of the copolymers were determined by gel permeation chromatography using tetrahydrofuran as a solvent with on a Waters 515-410 system (Waters, USA).

2.4. Copolymerization of CO2 and propylene oxide

Several copolymerization experiments were conducted in a 130 mL autoclave to evaluate the catalytic performance of the catalysts. The autoclave was loaded with a catalyst, placed under vacuum at 25 °C and purged with N2 three times to allow for the removal of any moisture. The autoclave was then cooled to room temperature and charged with propylene oxide using a syringe before being pressurized with CO2 to the desired pressure. Upon completion of the reaction, the autoclave was cooled to room temperature and the CO2 released.

3. Results and discussion
3.1. FT-IR spectra

The C≡N groups in the FTIR spectra of Zn-Co DMC catalysts generally give strong stretching vibrations (νCN) around 2196 cm-1 following the coordination of t-BuOH, whereas the corresponding νCN value of pure Zn3[Co(CN)6]2 is 2185 cm-1 [32]. As shown in Fig. 1, the FTIR spectra of CDMC1 and CDMC3 still contained a peak at 2195 cm-1 following the addition of 18-crown-6. Structural transformations of this type are generally thought to originate from the effective coordination of Zn with O for the polymerization process. Notably, the stretching vibration of the Co-C bond in pure Zn3[Co(CN)6]2 (DMC0), which is generally observed at 451 cm-1, was appeared at 471 and 472 cm-1in CDMC1 and CDMC3, respectively. Furthermore, the peaks at 1107 and 1109 cm-1in CDMC1 and CDMC3 were attributed to the stretching vibrations of the C-O-C bonds of 18-crown-6. Although different amounts of 18-crown-6 were added to CDMC1 and CDMC3, the IR curves of these materials were almost identical except for minor differences in the stretching vibrations of the C-O-C and Co-C bonds.

Fig. 1. FTIR spectra of CDMC1 (1), CDMC3 (2) and DMC0 (3).

The FTIR data for the stretching vibrations of the C≡N, Co-C and C-O-C bonds of the CDMC and DMC catalysts are shown in Table 2. These results revealed that the FTIR spectra of the top and bottom surfaces of CDMC1 and CDMC3 cakes, which were prepared with a crown ether to K+ molar ratio of 2:1, were the same. This indicated that the cakes of the CDMC1 and CDMC2 materials were totally uniform in terms of their composition. In contrast, the FTIR spectra of the top and bottom surfaces of the DMC1 and DMC2 cakes, which were prepared without any crown ether, revealed that the peaks corresponding to the stretching vibrations of the C≡N bonds were different, which indicated that the materials were unevenly distributed in terms of their composition. Polymers containing ether groups [e.g., poly(tetramethylene ether glycol) and polyethylene glycol] can be used as complexing agents to improve the activity of DMC catalysts [32, 33]. For the CDMC catalysts, it was envisaged that the addition of 18-crown-6 would not only lead to the binding of the K+ but that it would also coordinate Zn2+. In this way, the 18-crown-6 could perform as a co-complexing agent, which could improve the homogeneity of the catalysts. FTIR analysis of CDMC3 revealed stretching vibrations for the C-O-C bonds of the 18-crown-6 at 1107 cm-1, whereas the corresponding band appeared at 1109 cm-1 in CDMC1. This result therefore illustrates the differences in the complexation states of the different catalysts. In fact, the stretching vibrations of the Co-C bonds in all of the catalysts prepared in the current study except for DMC0 were in the range of 471-472 cm-1. The similarity in these values could be attributed to the Co-C bonds being positioned inside of the molecules so that they would not be affected by changes in the chemical environment. In summary, these results show that the addition of 18-crown-6 led to significant improvements in the homogeneity of catalysts.

Table 2
IR wavenumber data of νCN, νCo-C and νC-O-C in Zn-Co DMC catalysts.
3.2. SEM results

The surface morphologies of the different catalysts were clearly observed by SEM (Fig. 2). The surface of the CDMC3 catalyst prepared in the presence of the crown ether was relatively dispersive with a large surface area. For the CDMC3-T and CDMC3-B catalysts, their surfaces were disordered and multilayered, which indicated that the CDMC3 was even. However, the surface structures of the top and bottom portions of the DMC1 and DMC2 catalysts were found to be different, which indicated that these materials were not uniform, were consistent with those of the FTIR spectra.

Fig. 2. SEM images of CDMC3-T (a), CDMC3-B (b), CDMC3-T (c), CDMC3-B (d), DMC1-T (e), DMC1-B (f), DMC2-T (g) and DMC2-B (h).
3.3. TGA-IR results

TGA-IR spectra of the thermal decomposition products resulting from CDMC1 and DMC1 were recorded at different stages of the heating process to confirm the binding states of the t-BuOH and crown ether ligands in these systems based on weight loss, and the results are shown in Table 3.

Table 3
Thermal decomposition stages of DMC1 and CDMC1.

The decomposition profiles of DMC1 and CDMC1 were divided into three stages. The first of these stages occurred from 20 to about 120 °C. DMC1 and CDMC1 contained peaks at 3670, 2960, 1375 and 1059 cm-1, which were assigned to the νO-H, νC-H, νC-H and νC-O vibrations of t-BuOH (Fig. 3). These results indicated that free H2O and t-BuOH were being released during the first stage of the thermal decomposition process.

Fig. 3. FTIR spectra of gas mixture derived from thermal decomposition of DMC1 (a) and CDMC1 (b). (1) 94 °C; (2) 206 °C; (3) 326 °C; (4) 500 °C; (5) 625 °C. (c) TGA curves of DMC1 (1) and CDMC1 (2).

The second stage of the thermal decomposition process occurred from 120 to about 360 °C and corresponded to the loss of coordinated ligands (i.e., t-BuOH and/or 18-crown-6). The presence of an alkene analogue was confirmed by FTIR analysis, which revealed peaks at 3080 and 1646 cm-1 corresponding to ν=C-H and νC=C at 123 °C above. Further evidence of an alkene was provided by an increase in the intensity of the characteristic peaks of the alkene above 326 °C, as shown in Fig. 3(a). The t-BuOH molecules present in the DMC1 and CDMC1 catalysts would undergo a dehydration reaction during the second stage to give 2-methylprop-1-ene. Figure 3 also revealed the formation of peaks at 1149 and 1021 cm-1, which were assigned to the asymmetrical and symmetrical stretching vibration of the ether bond of the crown ether.

The final stage in the thermal decomposition profiles of the DMC1 and CDMC1 catalysts occurred from 360 to 770 °C. This stage was attributed to the decomposition of the cyano groups and the other organic ligands (i.e., t-BuOH and 18-crown-6) attached to the active metallic center. The change in the stretching vibration of the C≡N bond (2278 cm-1) in Fig. 3(a) (curve 4) implied that the cyano group was being converted to free cyanide during the final stage of the thermal decomposition process. At the same time, the characteristic adsorption peaks (3278 and 2180 cm-1) of an alkyne could also be seen. The decomposition residues of the DMC1 and CDMC1 catalysts were determined to be metallic oxides with weight ratios of 44.0% and 40.2%, respectively. The compositions of these metal oxides were found to be in agreement with the results of the elemental analysis (CDMC1: 21.6% Zn, 8.1% Co and 1.2% K; DMC1: 25.1% Zn, 8.6% Co and 1.4% K).

As shown in Table 3, the metal oxides composition of CDMC1 (about 40.2%) was less than that of DMC1 (about 44%) because of the extra crown ether co-complexing agents. The decomposition products of the organic ligands (alkene and alkyne) could be observed by FTIR until the temperature reached 750 °C, which indicated that these ligands were coordinated to the metal center. After 290 °C, the weight of the CDMC1 material diminished rapidly, whereas the weight loss from the DMC1 catalyst occurred at a much slower rate (Fig. 3 (c)). This difference in the weight loss profiles of the two catalysts could be attributed to the highly dispersive structure of CDMC1 compared with the more compact DMC1, as shown in Fig. 2. Furthermore, the loss of the cyano ligand from the CDMC1 material at 390 °C occurred at a much higher temperature than that of the DMC1 catalyst (357 °C). This difference was attributed to an enhanced level of coordination from the O atom of the crown ether to the Zn ion in the CDMC1 catalyst, which would have led to the weakening of the bond between the cyano group and Zn ion, whilst strengthening the interaction between the cyano group and the Co metal center. The overall weight loss from the CDMC1 material (59.2%) was higher than that of the DMC1 catalyst (56.0%) between 20 and 770 °C because of the complexation of the crown ether.

3.4. XRD analysis

The XRD patterns of all of the catalysts are shown in Fig. 4. As expected, DMC0 catalyst (pure Zn3[Co(CN)6]), prepared in the absence of the ligand and excess ZnCl2 contained sharp peaks with d-spacing values of 5.75, 5.07, 3.59, 2.54, and 2.28 Å, and exhibited a typical cubic lattice structure [36]. In general, the addition of an organic ligand such as t-BuOH can disrupt the crystal structure and lead to a reduction in the crystallinity [32], which would be consistent with our XRD results. Regardless of whether the crown ether was added or not, other CDMC and DMC catalysts contained very broad and highly dispersed signals, which implied rather weak crystalline structures. For example, the XRD pattern among CDMC1 catalysts was the flattest of the all of the catalysts most likely because it contained the largest amount of crown ether. The signals at 12° and 21° in the DMC1 and DMC2 increased gradually, which suggested that the inclusion of multiple washing steps was leading to the generation of a new crystalline phase.

Fig. 4. XRD patterns of the CDMC and DMC catalysts.
3.5. The reproducibility of the CDMC catalysts

CDMC2-1, CDMC2-2 and CDMC2-3 were prepared in the same manner using 18-crown-6 as the CDMC2. As shown in Table 4, the Zn/Co molar ratios of these materials varied slightly from 1.77% to 1.86% for three independent experiments. The C and N contents of these catalysts were found to be almost equal because of the robust and highly reproducible nature of the processes involved in the preparation of these catalysts.

Table 4
Elemental analyses of the CDMC catalysts.
3.6. Analysis of the polymerization results

The coupling reactions of CO2 and epoxides can occur under mild conditions [38]. The coupling and copolymerization of CO2 and propylene oxide can occur simultaneously according to Scheme 1. The amount of the copolymer and the coupling product can be counted by 1H-NMR as shown in Fig. 5. The presence of K+ in catalysts can have an adverse impact on their selectivity. 18-Crown-6 was used to coordinate to the K+ in an attempt to simply the procedure for the synthesis of uniform active heterogeneous Zn-Co DMC catalysts, which appear to provide the most promising combination of metals with high levels of activity and selectivity in copolymerization reactions. The results in Table 5 clearly show that the CDMC1 catalyst showed catalytic activity as high as 21889 g/g Zn, which was much higher than those of the DMC1 and DMC2 catalysts (16300 and 16400 g/g Zn, respectively). The polymer prepared in the presence of CDMC3 had a similar carbonate linkage content (47.8%) to that of DMC2 (48.3%), but much higher catalytic activity (32600 g/g Zn). The DMC1 catalyst prepared without 18-crown-6 and more washing steps, which was shown to contain 1.43% K by ICP analysis, was less active and selective than all of the CDMC catalysts and the DMC2 catalyst with seven washing steps. These results therefore imply that the free K+ would be harmful to the copolymerization reactions of CO2 and epoxides. No K+ was detected in the DMC2 catalyst. Both of the CDMC1 and CDMC2 materials were found to be much more active than DMC1. This result indicated that the coordination of the K+ to 18-crown-6 was beneficial to the copolymerization reaction. DMC0, which was prepared without any organic ligands, had hardly any activity, which indicated that an active metallic center must be formed between a metal and some organic ligands to allow for the copolymerization of CO2 with epoxides.

Table 5
Results of the copolymerization catalyzed by various DMC catalysts a.

Scheme 1. Synthesis of PPC.

Fig. 5. 1H NMR spectrum of the PPC copolymer.
3.7. Possible mechanism

Several well-known DMC catalysts have been used during the past two decades to catalyze the polymerization reactions of epoxides and the copolymerization reactions of CO2 with epoxides. Once the long induction time or activation stage is over, the polymerization reaction will proceed rapidly and reach termination in a short time. The final product of these reactions has two hydroxyl end groups, as confirmed by Zhang et al. [33]. It was envisaged that the polymerization reaction described in the current study proceeded in two stages, the slow activation stage and the rapid propagation stage, as depicted in Scheme 2. The reaction would begin with the coordination of PO to Zn and the subsequent nucleophilic ring-opening of the PO by a hydroxyl group coordinated to the active Zn center. Given that the amount of catalyst would be small relative to the monomer, the hydroxyl group coordinated to the active Zn center would not be regenerated, and the speed of the activation stage would therefore be restricted. However, during the propagation of the intermediate, the resulting Zn-OR species could trigger a further polymerization reaction and be regenerated through a chain transfer, which would lead to the auto acceleration of the polymerization process. In addition, Lee et al. [39] found that the use of small linear aliphatic alcohols was preferred over bulky t-BuOH in terms of shortening the induction period. It is possible that the reduction in steric hindrance resulting from the use of smaller alcohols would lead to an increase in the chain transfer, and therefore accelerate the activation period .

Scheme 2. Proposed mechanism of copolymerization.
4. Conclusions

18-Crown-6 has been used for the first time to coordinate K+ in an attempt to generate uniform and highly active Zn-Co DMC catalysts. Based on the FTIR and SEM results, it was clear that the addition of crown ether had a significant impact on the surface morphologies of the catalysts, which became even and uniformly dispersed compared to the layered and compacted surfaces of the catalysts prepared in the absence of the crown ether. TGA-IR analysis showed that the active metallic center was formed from several metals coordinated to organic ligands (t-BuOH and 18-crown-6). In spite of the large excess of K+, the crown ether complexing Zn-Co DMC catalyst prepared without the inclusion of extra washing steps (CDMC1) showed a high catalytic efficiency, which was similar to that the DMC2 catalyst prepared with multiple washings but in the absence of the crown ether. The catalytic efficiency of this material as high as 5122 g/g catalyst (32600 g/g Zn) was obtained in the presence of a Zn-Co DMC with the addition of double the theoretical amount of the crown ether.

References
[1] Muelhaupt R. Macromol Chem Phys, 2013, 214: 159
[2] Nornberg B, Borchardt E, Luinstra G A, Fromm J. Eur Polym J, 2014, 51: 167
[3] Tang R Z, Chen T, Chen Y, Zhang Y Z, Wang G Y. Chin J Catal (唐荣芝, 陈彤, 陈勇, 张元卓, 王公应. 催化学报), 2014, 35: 457
[4] Liu J, Wang A Q, Jing H W. Chin J Catal (刘靖, 王安琪, 景欢旺. 催化学报), 2014, 35: 1669
[5] Kuran W, Listos T. Macromol Chem Phys, 1994, 195: 977
[6] Darensbourg D J, Holtcamp M W, Struck G E, Zimmer M S, Niezgoda S A, Rainey P, Robertson J B, Draper J D, Reibenspies J H. J Am Chem Soc, 1999, 121: 107
[7] Kim J S, Kim H, Yoon J, Heo K, Ree M. J Polym Sci Part A Polym Chem, 2005, 43: 4079
[8] Tang L, Xiao M, Xu Y, Wang S J, Meng Y Z. J Polym Res, 2013, 20: 190
[9] Meng Y Z, Du L C, Tiong S C, Zhu Q, Hay A S. J Polym Sci Part A Polym Chem, 2002, 40: 3579
[10] Olejnik R, Padelkova Z, Fridrichova A, Horacek M, Merna J, Ruzicka A. J Organomet Chem, 2014, 759: 1
[11] Pan X, Liu Z, Cheng R H, Jin D L, He X L, Liu B P. J Organomet Chem, 2014, 753: 63
[12] Dong Y L, Wang X H, Zhao X J, Wang F S. J Polym Sci Part A Polym Chem, 2012, 50: 362
[13] Wu W, Qin Y S, Wang X H, Wang F S. J Polym Sci Part A Polym Chem, 2013, 51: 493
[14] Anderson C E, Vagin S I, Hammann M, Zimmermann L, Rieger B. ChemCatChem, 2013, 5: 3269
[15] Bai D S, Wang X X, Song Y Y, Li B, Zhang L L, Yan P, Jing H W. Chin J Catal (柏东升, 王晓旋, 宋莹莹, 李博, 张立龙, 闫鹏, 景欢旺. 催化学报), 2010, 31: 176
[16] Cheng M, Lobkovsky E B, Coates G W. J Am Chem Soc, 1998, 120: 11018
[17] Zhang M, Chen L B, Liu B H, Yan Z R, Qin G, Li Z M. Polym Bull, 2001, 47: 255
[18] Rajendran N M, Haleel A, Reddy N D. Organometallics, 2014, 33: 217
[19] Wu G P, Xu P X, Lu X B, Zu Y P, Wei S H, Ren W M, Darensbourg D J. Macromolecules, 2013, 46: 2128
[20] Lu X B, Ren W M, Wu G P. Acc Chem Res, 2012, 45: 1721
[21] Darensbourg D J, Chung W C, Wilson S J. ACS Catal, 2013, 3: 3050
[22] Enthaler S. ACS Catal, 2013, 3: 150
[23] Tsai C Y, Huang B H, Hsiao M W, Lin C C, Ko B T. Inorg Chem, 2014, 53: 5109
[24] Nakano K, Kobayashi K, Ohkawara T, Imoto H, Nozaki K. J Am Chem Soc, 2013, 135: 8456
[25] Xie Y, Wang T T, Liu X H, Zou K, Deng W Q. Nat Commun, 2013, 4: 1960
[26] Oh H J, Ko Y S. J Ind Eng Chem, 2013, 19: 1939
[27] Huang Y J, Qi G R, Chen L S. Appl Catal A, 2003, 240: 263
[28] Chen S, Hua Z J, Fang Z, Qi G R. Polymer, 2004, 45: 6519
[29] Varghese J K, Park D S, Jeon J Y, Lee B Y. J Polym Sci Part A Polym Chem, 2013, 51: 4811
[30] Sebastian J, Srinivas D. Appl Catal A, 2014, 482: 300
[31] Zhou T C, Zou Z Q, Gan J Q, Chen L B, Zhang M. J Polym Res, 2011, 18: 2071
[32] Zhang X H, Hua Z J, Chen S, Liu F, Sun X K, Qi G R. Appl Catal A, 2007, 325: 91
[33] Zhang X H, Wei R J, Sun X K, Zhang J F, Du B Y, Fan Z Q, Qi G R. Polymer, 2011, 52: 5494
[34] Kim I, Yi M J, Lee K J, Park D W, Kim B U, Ha C S. Catal Today, 2006, 111: 292
[35] Ravindran A, Srivastavas R. Chin J Catal (催化学报), 2011, 32: 1597
[36] Kim I, Ahn J T, Ha C S, Yang C S, Park I. Polymer, 2003, 44: 3417
[37] Chen S, Zhang X H, Qi G R. Chin J Catal (陈上, 张兴宏, 戚国荣. 催化学报), 2006, 27: 355
[38] Chang T, Gao X R, Bian L, Fu X Y, Yuan M X, Jing H W. Chin J Catal (常涛, 高晓蕊, 边丽, 付西英, 袁明霞, 景欢旺. 催化学报), 2015, 36: 408
[39] Lee S H, Lee I K, Ha J Y, Jo J K, Park I, Ha C S, Suh H, Kim I. Ind Eng Chem Res, 2010, 49: 4107